Dry-Process Rubber Asphalt for the Midwest

No blending unit. No reaction tank. Rubber goes straight into the drum with the aggregate. Dry process is the easiest way for a Midwest plant to start using ground tire rubber, and the math is simple.

Freshly paved rubberized asphalt highway through Midwest farmland

Three ways rubber gets into asphalt

The FHWA's 2020 tech brief The Use of Recycled Tire Rubber to Modify Asphalt Binder and Mixtures (FHWA-HIF-20-043) describes three main routes for ground tire rubber (GTR):

Process Where the rubber goes GTR level (FHWA) Typical GTR size (FHWA)
Wet process, field blend (asphalt rubber) Blended and reacted with hot binder at the plant 10-22% by weight of binder Max ~1.5 mm (15 mesh)
Wet process, terminal blend Blended at the terminal, shipped as binder 5-15% 30-80 mesh, 30-40 most typical
Dry process Added with aggregate into the mixing drum ~10% by weight of binder 30-40 mesh

Field-blend asphalt rubber is a western staple (Arizona, California). Terminal blend lives at the binder terminal. Dry process is the one a hot-mix plant can run with the equipment it already has, plus a way to meter the rubber.

Freshly paved rubberized asphalt highway through Midwest farmland
A finished dry-process mat looks and paves like conventional hot mix.

How the dry process works

  1. GTR arrives at the plant. FHWA notes GTR is delivered "in bulk or super-sacks."
  2. It's metered into the drum or pugmill, usually through a dedicated feeder or the plant's fiber/RAP collar, at a set rate per ton of mix.
  3. It mixes with hot aggregate before or with the binder.
  4. Some systems use engineered (pre-treated) GTR with additives to help the rubber interact with the binder during mixing, storage and haul.
  5. Paving and compaction are similar to conventional mix, following the agency's spec.

The math

FHWA says dry-process GTR is typically about 10% by weight of binder, which works out to roughly 0.5% by weight of the mix at typical binder contents, or about 10 lb of rubber per ton of mix.

Example 1: A 10,000-ton overlay

  • 10,000 tons × 10 lb/ton = 100,000 lb of GTR
  • About 50 supersacks (2,000 lb), or 2.5 truckloads
  • Spread over a 10-day paving window: 10,000 lb a day, about 5 sacks

Example 2: Check it against binder content

A mix at 5.5% binder: - Binder per ton = 2,000 × 5.5% = 110 lb - GTR at 10% of binder = 11 lb per ton - 0.55% of the mix, consistent with FHWA's "about 0.5%"

At 5.0% binder you'd be at 10 lb/ton. Run your own mix design numbers.

Example 3: A season of production

A plant running 60,000 tons of rubber-modified mix in a season at 10 lb/ton needs 600,000 lb of 30-minus, about 300 sacks or 14-15 truckloads. That's well inside what we keep in stock. Schedule loads weekly so the yard never runs dry.

Where it's been used

FHWA's brief reports dry-process GTR projects since 2007 in states including Georgia, Illinois, Indiana, Louisiana, Maryland, Missouri, Oklahoma, Texas, Virginia and Wisconsin, and notes "dry-mix" projects in Michigan and Ohio. That's the Midwest, and it's within a day's haul of Central Ohio.

Every state handles GTR differently: some through special provisions, some through standard specs, some by project-by-project approval. Before you bid, get the agency's current provision and its GTR requirements. Specs change; we'll read yours with you.

Bidding a GTR job? Get 30-minus priced delivered to your plant. Send grade, volume, delivery city/ZIP and your target price.

Request a Quote

Why the mesh matters

Dry process wants fine rubber, and FHWA's 30-40 mesh range is the target. Finer particles disperse better in the mix and have more surface to interact with the binder. That's exactly what our 30-minus is: everything passes the No. 30 screen (600 µm). For specs calling for 40 mesh, we make 40 mesh to order.

Under ASTM D5603, a "30 mesh" grade has zero retained on No. 20 and no more than 10% retained on No. 30, tested by ASTM D5644. If your provision names a gradation band, we test to it.

What contractors and QC need

  • Gradation to the spec band, with a lot sieve report
  • Residual steel and fiber limits (rubber with steel or fiber balls clogs feeders)
  • Moisture, typically ≤1%, so it meters smoothly
  • Specific gravity if the spec calls for it
  • Certificates of tire origin where required
  • Consistent lots across the season so your mix design holds

Plant setup tips

  • Feeder calibration. Calibrate the GTR feeder at the start of each run. 10 lb a ton is a small stream; a few pounds off is a big percentage.
  • Sack handling. Supersacks lift by their loops with a forklift. Keep a dry staging area near the feeder.
  • Dust. Fine rubber is light. Use the plant's dust controls and discharge spouts.
  • Records. Log GTR used per ton for the agency.

The upside

  • No blending unit or reaction tank needed
  • Uses tire rubber that would otherwise go to fuel or disposal
  • Fits standard paving operations
  • Gives agencies a GTR option they can specify on ordinary projects

A first-project roadmap for a hot-mix producer

If your plant has never run GTR, the first job feels like a big step. It doesn't have to be. A practical sequence:

  1. Read the agency's provision and note the GTR gradation, dose, any pre-treatment requirement, mixing temperature and any extra mixing or "digestion" time.
  2. Work with your mix designer to run the design with the specified GTR. The rubber dose is set by weight of binder, so binder content and rubber dose are linked.
  3. Line up supply early. Confirm the supplier can deliver consistent lots for the whole job, with sieve reports on each.
  4. Set up and calibrate the feeder. A small, steady stream of rubber needs accurate metering.
  5. Run a trial batch and check the mix against the design before production.
  6. Plan storage at the plant. Supersacks need a dry area close to the feeder, with forklift access.
  7. Keep good records of GTR used per ton and per day for the agency.

Questions to ask your rubber supplier

  • What's the gradation of the material you'll ship, and how often do you test it?
  • What are your typical residual steel, fiber and moisture numbers?
  • Can you supply the whole job from consistent production?
  • How much do you keep in stock, and how fast can a truck leave after I call?
  • Will you ship supersacks with or without pallets, and with discharge spouts if my feeder needs them?

What can go wrong, and how to avoid it

  • Feeder bridging. Fine rubber can bridge in a hopper. Use the right feeder, keep the rubber dry and avoid fiber balls.
  • Inconsistent dosing. Calibrate often and log feeder rates.
  • Wet rubber. Moisture makes metering unreliable. Store covered.
  • Mix temperature and time. Follow the provision. Rubber needs time and heat to interact with the binder.
  • Running out mid-job. Order ahead and keep a few days of rubber on site.

With a good supplier and a calibrated feeder, the dry process lets a Midwest plant add GTR mixes to its lineup without major capital spending.

Dry process vs wet process: choosing the right route

Owners and contractors often ask which process is "better." The honest answer is that they solve different problems:

Question Dry process Wet process (field blend) Terminal blend
New plant equipment? Usually just a feeder Blending and reaction unit None at the plant
Where's the rubber dosed? Into the mix Into the binder at the plant Into the binder at the terminal
Typical GTR level (FHWA) ~10% of binder 10-22% of binder 5-15% of binder
Typical size (FHWA) 30-40 mesh Up to ~15 mesh 30-80 mesh
Who buys the rubber? The mix producer The AR binder contractor The binder supplier

For a Midwest producer, the dry process is often the most practical way to start, because the rubber goes in like any other additive. Where an agency calls for asphalt rubber binder with a high rubber content, the wet process is the established route. Terminal blends let a producer use rubber-modified binder delivered like any other liquid asphalt.

Whichever route your project takes, the rubber still has to be clean, dry and consistently graded. That's the part we handle.

Seasonal timing

Paving in the Midwest runs from spring to late fall, and lettings cluster in the winter and early spring. That timing matters for rubber supply. Lining up a supplier when bids are being prepared, rather than after award, lets you quote with a firm delivered price and confirmed availability. Ask for a sample and lot data early so your mix designer has time to run the design with the actual rubber you'll use.

Frequently asked questions

How much crumb rubber goes in a ton of dry-process asphalt?

FHWA puts it at about 10% of binder weight, around 0.5% of the mix, or roughly 10 lb per ton.

What mesh is used for dry process?

FHWA says 30-40 mesh is typical. Our 30-minus is the usual pick; 40 mesh is made to order.

Do I need special equipment?

Usually a metering feeder. No blending or reaction unit is needed.

Which Midwest states have used it?

FHWA lists Illinois, Indiana, Missouri and Wisconsin among dry-process states, plus dry-mix projects in Michigan and Ohio.

Can you ship to my plant weekly?

Yes. We schedule recurring loads in supersacks.

Sources: FHWA, The Use of Recycled Tire Rubber to Modify Asphalt Binder and Mixtures, FHWA-HIF-20-043, 2020 (PDF); ASTM D5603-19a; ASTM D5644-23.

Need crumb rubber
by the truckload?

Send your grade, quantity and delivery ZIP or export destination. We'll review availability, packaging and freight, then come back with a written quote.

Request a Quote CallEmail