Request a Quote
Guide · Quality

Crumb Rubber Specs Explained

Every line on a crumb rubber spec sheet exists because somebody once got a bad load. Here's what each one means, what standard it ties to, and what to ask for.

Lab technician weighing crumb rubber retained on a test sieve beside a sieve shaker

The two ASTM standards every buyer should know

  • ASTM D5603, Standard Classification for Rubber Compounding Materials—Recycled Vulcanizate Rubber. It classifies recycled rubber by particle size and by source (the parent material, from whole tires to tread-only to non-tire rubber). ASTM notes this material is used for "synthetic turf infill, asphalt-rubber, molded rubber products, tire-derived fuel, and other tire and non-tire derived products."
  • ASTM D5644, Standard Test Method... Determination of Particle Size Distribution of Recycled Vulcanizate Particulate Rubber. It's the sieve-shaker (Ro-Tap style) method for particles 90 µm (170 mesh) or larger.

Agencies often layer their own requirements on top. ADOT's asphalt-rubber spec, for example, has set rubber specific gravity at 1.15 ± 0.05 and fabric limits of 0.1% or 0.5% depending on type.

Line by line

Nominal size / mesh designation

The label: 10-20, 30-minus, 40 mesh. Under D5603 it's defined by a zero screen (0% retained) and a designation screen (≤5%, ≤10% or ≤15% retained depending on size). See the mesh size guide.

Sieve distribution

The full curve: percent retained on each screen. This is the line that matters most. Ask for it per lot.

Residual steel (metal)

Tire wire left after magnetic separation. Steel damages molds, knives and pumps, and shows up in finished goods. Fine grades are usually held to very low limits; coarse grades may be allowed more. Our sheets show production targets and typical values, confirmed per lot.

Fiber

Tire cord (polyester, nylon) left after air separation. Fiber balls ruin sealant finishes and mat faces. ADOT's asphalt-rubber spec has allowed only 0.1% fabric for Type A and 0.5% for Type B.

Moisture

Crumb rubber is hydrophobic but can pick up surface moisture in storage. Moisture foams hot asphalt and reacts with isocyanate (polyurethane) binders. Set a limit.

Specific gravity

Tire rubber is denser than water. ADOT has specified 1.15 ± 0.05 for asphalt-rubber crumb. Our sheets list typical ~1.15.

Source / classification

Whole tire, passenger vs. truck, tread only, etc. Matters for polymer content (natural vs. synthetic rubber) and consistency. Caltrans, for example, requires a separate high natural rubber CRM component (25% ± 2% of the CRM) in its asphalt rubber.

Contaminants and parting agents

Stones, glass, non-ferrous metal and dust. Some specs allow anti-caking agents: ADOT has allowed up to 4% calcium carbonate by weight of the rubber.

Packaging, lead time, minimum order

Not quality items, but they're on the sheet for a reason. Ours: supersacks with or without pallets, typical ~2,000 lb net; in-stock grades ship fast; made-to-order lead times confirmed at quote.

Conveyor feeding ground rubber into a vibrating screener inside a crumb rubber plant
Screening is where the sieve curve is made, and it's where good suppliers control it.

Typical vs. guaranteed

Spec sheets mix two kinds of numbers:

  • Typical / representative: what production usually looks like
  • Guaranteed / max-min: what the lot must meet to be accepted

Ours mark typical values clearly. Your purchase order should state the guaranteed limits you need, the test method, and what happens if a lot misses.

What a lot COA should include

  1. Lot or bag ID and production date
  2. Sieve distribution by ASTM D5644 (screens agreed in advance)
  3. Residual steel and fiber results
  4. Moisture
  5. Source/classification statement
  6. Any agency-specific items (specific gravity, etc.)

Worked example: writing a tight PO spec

A molder's spec for 10-20 mesh

  • Size: 10-20 mesh; 0% retained on No. 8; ≤5% retained on No. 10; ≤10% passing No. 30 (test: ASTM D5644)
  • Residual steel: per agreed max, by magnet test on 100 g
  • Fiber: per agreed max, visual/weight method agreed in advance
  • Moisture: ≤1.0%
  • Source: whole tire crumb, statement on COA
  • Packaging: supersack without pallet, ~2,000 lb net, labeled with lot ID
  • Acceptance: COA with each load; buyer may retain a sample per sack

That spec leaves nobody guessing.

Send us your spec, we'll match a lot. Send grade, volume, delivery city/ZIP and your target price.

Request a Quote

Frequently asked questions

What is ASTM D5603?

The standard classification for recycled vulcanizate rubber, by particle size and source.

What is ASTM D5644?

The test method for particle size distribution of recycled rubber by vibratory sieve shaker, for particles 90 µm and larger.

What's an acceptable steel content?

It depends on your application. Set a number, a test method, and ask for it on every COA.

Why does moisture matter?

It foams hot asphalt and reacts with polyurethane binders.

Do you provide COAs?

Yes, lot data is available on request with your quote.

Sources: ASTM D5603-23 and D5644-23 (astm.org); ADOT §1009 as reproduced in Summary of Rubber Modified Asphalt Product Specifications around the World (2012); Caltrans Construction Manual §4-39.

Need crumb rubber
by the truckload?

Send your grade, quantity and delivery ZIP or export destination. We'll review availability, packaging and freight, then come back with a written quote.

Request a Quote CallEmail